Suhm Spring Works - Materials Properties
Material |
Material
Properties |
Maximum
Working Temp. |
|
Modulus
of Elasticity |
Approx.
Design % of Ultimate Tensile (torsional) |
Common
Sizes, |
Titanium
Beta-C |
Age
hardened. Good ductility and toughness.
Good fabricability, and good resistance to
general corrosion. Good for environments
containing Ferric Chloride, Sodium Chloride,
Carbon Dioxide, and Hydrogen Sulfide |
600°F |
190/180 |
(E) 15.4 (G)
5.9 |
45% |
.005" to .625" |
Wire Diameter, in |
|||||||
.005 |
.014 |
.025 |
.062 |
.125 |
.187 |
.312 |
.562 |
.007 |
.015 |
.032 |
.072 |
.135 |
.192 |
.343 |
.625 |
.008 |
.017 |
.045 |
.080 |
.148 |
.207 |
.375 |
|
.009 |
.018 |
.048 |
.093 |
.156 |
.225 |
.406 |
|
.010 |
.021 |
.050 |
.105 |
.162 |
.243 |
.437 |
|
.012 |
.022 |
.054 |
.114 |
.177 |
.250 |
.500 |
VALUES
INDICATE COLD DRAWN AND AGED MATERIAL
Nominal Diameter, inches |
Tensile
Strength, psi |
Elongation in 4D %, minimum |
Reduction
of Area %, min. |
Up
to 0.187,
incl. |
190,000
- 210,000 |
10 |
20 |
Over
0.187 to 0.375 incl. |
185,000
- 205,000 |
10 |
20 |
Over
0.375 to 0.625 incl. |
180,000
- 200,000 |
8 |
20 |
COMMENTS: |
Material has been cold drawn 20 - 35% final reduction. Additional cold reduction may be possible to produce higher tensile/yield strength. Larger sizes can be obtained in spring tempered and annealed condition. Check with a Suhm representative for size and tensile strengths. |
These data are provided as a reference guide only and are not intended for design purposes. Strength values and sizes are subject to change. Please check with a Suhm Spring representative for confirmation.